Air permeability testing of corrugated base paper (corrugating medium) quantifies how easily air passes through the sheet under a controlled pressure differential, providing critical insight into fiber furnish, refining, formation, and converting performance. This technical guide explains the testing principle, applicable ISO, GB, and TAPPI standards, sample preparation requirements, instrument methods, and practical applications for paper mills and corrugated packaging manufacturers.
Technical Overview
Air permeability, more precisely termed air permeance, describes the volume of air that passes through a defined area of paper per unit time under a specified pressure difference. For corrugated base paper (corrugating medium), the property is governed by the internal pore structure of the sheet, which in turn reflects fiber type, refining intensity, pressing and drying conditions, filler content, and the degree of sizing or impregnation. The general relationship is expressed as permeance P = V / (A × t × Δp), where V is the air volume, A the measurement area, t the time, and Δp the applied pressure difference.
Corrugated base paper is a relatively porous, unsized or lightly sized engineering material, so its permeance typically falls in the medium range covered by the ISO 5636 series of methods. The value is important to converters because permeability influences heat and steam transfer during fluting on the single facer, adhesive penetration at the glue line, moisture migration and warp tendency, and the behavior of the sheet on vacuum-assisted transfer sections of high-speed corrugators. Depending on the method, results are reported in μm/(Pa·s), mL/min, or seconds per 100 mL, and these units are not directly interchangeable without conversion of both flow area and driving pressure.
Air permeability testing of corrugated base paper is commonly performed as a supplementary quality index agreed between supplier and purchaser, alongside mandatory strength properties such as ring crush strength, Concora medium test (CMT), bursting strength, and grammage specified in product standards such as GB/T 13023 for corrugated medium.
Testing Samples
Sample Types and Grades
Test material is typically corrugating medium taken from production rolls or cut sheets, covering the full commercial grammage range of approximately 80 g/m² to 200 g/m². Samples may represent different commercial grades, semi-chemical corrugating medium, or recycled-furnish medium, and both machine-made rolls and laboratory-prepared handsheets can be evaluated for research purposes. Because the sheet is frequently two-sided (wire side versus felt side), the tested face must be recorded.
Sampling Requirements
Sampling follows ISO 186 or GB/T 450, taking test pieces from positions representative of the whole lot while avoiding damaged edges, folds, wrinkles, watermarks, and visible defects. For the Schopper method, test pieces of approximately 60 mm × 100 mm are customary, providing adequate margin around the standard 10 cm² clamping aperture. At least ten valid test pieces are recommended, alternating the tested side so that two-sidedness is captured in the reported data.
Conditioning
All test pieces must be conditioned to equilibrium in the standard atmosphere specified in ISO 187 or GB/T 10739, that is, 23 °C ± 1 °C and 50% ± 2% relative humidity. This step is essential because the moisture content of the sheet measurably changes pore geometry and fiber stiffness, and therefore the measured permeance.
Testing Items
The primary measurable quantity is air permeance of corrugated base paper, with reporting options including:
- Air permeance by the Schopper method, expressed in μm/(Pa·s), per ISO 5636-2 / GB/T 458
- Air permeance by the Bendtsen method, expressed in mL/min, per ISO 5636-3 / GB/T 2679.13
- Air resistance by the Gurley method, expressed in seconds per 100 mL, per ISO 5636-5 / GB/T 5402 / TAPPI T 460
- Statistical treatment of results: arithmetic mean, maximum, minimum, standard deviation, and, where required, comparison against contractual specification limits
Testing Methods
General Principle
All medium-range methods clamp a conditioned test piece over a precision aperture, seal the edges, and draw or force air through the sheet at a controlled, constant pressure difference. Either the time for a fixed air volume is measured (constant-pressure, time-based methods such as Schopper and Gurley) or the steady-state flow rate is read directly (flow-based methods such as Bendtsen). Sealing quality, zero-leak verification, and calibration of the pressure and flow elements are prerequisites for valid results.
Schopper Method (ISO 5636-2 / GB/T 458)
The test piece is clamped over a 10 cm² opening on a water-sealed apparatus. As water is discharged from a sealed vessel, a negative pressure of nominally 1.33 kPa draws atmospheric air through the sheet, and the time required for 100 mL of air to pass is recorded. The result is converted to air permeance in μm/(Pa·s), which is numerically equal to mL/(m²·Pa·s). The Schopper method is the most widely referenced procedure for corrugated base paper in Chinese trade practice.
Bendtsen Method (ISO 5636-3 / GB/T 2679.13)
A steady stream of air at approximately 1.47 kPa (150 mm water column) is drawn through the 10 cm² measurement area, and the flow rate is read from a calibrated rotameter or electronic flow sensor. Results are reported in mL/min. The method is well suited to rapid in-plant quality control on medium-permeability grades.
Gurley Method (ISO 5636-5 / GB/T 5402 / TAPPI T 460)
A cylinder of known weight descends in sealing oil, displacing 100 cm³ of air through a 6.45 cm² (1 square inch) aperture at a pressure difference of approximately 1.2 kPa. The time in seconds for the full volume to pass is the Gurley air resistance. Because it measures resistance rather than permeance, a higher value indicates a denser, less permeable sheet.
Sheffield Method (ISO 5636-4)
The Sheffield procedure applies a different pressure and flow regime and reports flow on its dedicated scale. It is generally reserved for sheets whose permeance lies outside the comfortable range of the other instruments or when legacy specifications reference the method.
Calculation, Reporting, and Quality Assurance
Reports issued in accordance with ISO 5636-1 state the method and standard used, the instrument type, conditioning atmosphere, number of test pieces, mean permeance or resistance value, extreme values, standard deviation, tested side, and any deviations from the standard. Calibration against reference orifices, leak checks before each session, and participation in interlaboratory comparisons at accredited third-party laboratories ensure metrological traceability of the results.
Applications
Air permeability data for corrugated base paper support a wide range of industrial uses:
- Incoming inspection at corrugated box plants, verifying that purchased medium meets contract specifications before committing it to production
- Paper mill process control, tracing the effect of refining energy, furnish changes, pressing load, and drying profile on sheet structure
- Corrugator optimization, where permeability affects heat transfer at the hot plates and pressure rolls, glue penetration, bond formation, and warp control
- Lightweighting and recycled-content development programs, in which permeability is balanced against ring crush, CMT, and burst performance
- Failure analysis and supplier dispute resolution, using traceable test reports from accredited third-party laboratories
- Technical documentation for export shipments and customer audits where permeability is a contractual index
FAQ
Which method is most appropriate for corrugated base paper?
The Schopper method (ISO 5636-2 / GB/T 458) is the most common reference for corrugated base paper in Chinese commerce, while the Gurley method is frequently cited in international specifications. The choice should match the standard named in the purchase contract, because results from different methods cannot be compared directly.
What units are reported?
Schopper results are given in μm/(Pa·s), Bendtsen results in mL/min, and Gurley results in seconds per 100 mL. Note that Gurley values express air resistance, so they move in the opposite direction to permeance.
Why is conditioning so critical?
Moisture changes fiber swelling and pore dimensions in the sheet. Testing without equilibrium conditioning at 23 °C and 50% relative humidity produces biased, non-reproducible values.
Does higher permeability mean better quality?
Not inherently. Permeability must be balanced against strength properties such as ring crush, CMT, and burst, and against converting behavior on the corrugator. Very high permeability in a lightweight medium can indicate low density and reduced stacking strength, while extremely low permeability may impair heat and moisture transfer during fluting.
How many test pieces are required?
A minimum of ten valid determinations is recommended, alternating the wire side and felt side so that two-sidedness of the sheet is represented in the mean value and scatter statistics.
Why Choose ZKGX?
- State-of-the-art analytical equipment
- Highly qualified scientific team
- Fast turnaround time
- Competitive pricing