Ubicación: Global + English
Global Global Algérie Français Algeria English Angola Português Angola English Argentina Español Argentina English Australia English Austria Deutsch Austria English Azerbaijan English Azerbaijan Русский Bahrain English Bangladesh English Belgium English Belgium Français Belgium Nederlands Brazil Português Brazil English Bulgaria български Bulgaria English Cameroon English Cameroon Français Canada English Canada Français Chile Español Chile English China 中文 China 日本語 China English Colombia Español Colombia English Croatia English Czech Republic Čeština Czech Republic English Denmark English Djibouti English Ecuador Español Ecuador English Egypt English Estonia English Ethiopia English Finland Suomi Finland English France Français France English Georgia English Georgia Русский Germany Deutsch Germany English Ghana English Greece Ελληνικά Greece English Guatemala Español Guatemala English Hong Kong, China English Hong Kong, China 中文 Hungary Magyar Hungary English India English Indonesia English Iraq English Ireland English Italy Italiano Italy English Ivory Coast Français Ivory Coast English Japan 日本語 Japan English Jordan English Kazakhstan Русский Kazakhstan English Kenya English Kuwait English Kyrgyzstan Русский Kyrgyzstan English Latvia English Lithuania English Malaysia English Mauritius English Mauritius français (Maurice) Mexico Español Mexico English Moldova Română Moldova English Mongolia English Morocco English Morocco Français Mozambique Português Mozambique English Netherlands Nederlands Netherlands English New Zealand English Nigeria English Norway English Oman English Pakistan English Paraguay Español Paraguay English Peru Español Peru English Philippines English Poland Polski Poland English Portugal Português Portugal English Qatar English Republic of Korea 한국어 Republic of Korea English Romania Română Romania English Saudi Arabia English Serbia Српски Serbia English Singapore English Slovakia English Slovenia English South Africa English Spain English Spain Español Sri Lanka English Sweden English Switzerland Deutsch Switzerland Français Switzerland Italiano Switzerland English Tanzania English Thailand ไทย Thailand English Togo English Togo Français Tunisia English Tunisia Français Türkiye Türkçe Türkiye English Turkmenistan Русский Turkmenistan English Ukraine Українська Ukraine English United Arab Emirates English United Kingdom English Uruguay Español Uruguay English USA English Uzbekistan English Uzbekistan Русский Vietnam Tiếng Việt Vietnam English

Concrete Flexural Strength Test Procedure: A Complete Step-by-Step Laboratory Guide

The concrete flexural strength test, also known as the modulus of rupture test, is a fundamental laboratory procedure used to evaluate the ability of concrete beams to resist bending failure. This step-by-step guide explains the complete experimental procedure in accordance with international standards such as GB/T 50081, ASTM C78, ASTM C293, EN 12390-5, and ISO 1920-4, covering specimen preparation, apparatus setup, loading, calculation, and result validation. It is an essential reference for civil engineers, laboratory technicians, and quality-control professionals involved in concrete pavement, runway, and slab construction.

Technical Overview

Flexural strength, commonly referred to as the modulus of rupture, is the tensile stress at which a concrete beam fails under bending. Unlike compressive strength, which measures resistance to crushing, flexural strength reflects the performance of concrete in structures subjected to bending stresses, such as rigid pavements, airport runways, industrial floors, and slab-on-grade construction. Because concrete is weak in tension, flexural strength is typically only about 10% to 20% of its compressive strength, making it a critical design parameter for thin, plate-like concrete elements.

The test is performed by loading a prismatic beam specimen to failure using either third-point loading (four-point bending) or center-point loading (three-point bending). Third-point loading is the preferred method in most standards because it produces a zone of pure bending without shear between the two loading points, giving a more representative measure of true flexural capacity. The principal standards governing this test include GB/T 50081 (Standard for Test Methods of Physical and Mechanical Properties of Concrete), ASTM C78 (third-point loading), ASTM C293 (center-point loading), EN 12390-5, and ISO 1920-4. Tests should be carried out by accredited third-party laboratories or qualified in-house materials laboratories using calibrated loading frames and fixtures.

Testing Samples

Standard Prism Specimens

The standard specimen for the third-point loading flexural test is a prismatic beam. Under GB/T 50081, the standard dimensions are 150 mm × 150 mm in cross-section with a length of 550 mm to 600 mm, tested over a support span of 450 mm. ASTM C78 uses a beam of 152 mm × 152 mm × 508 mm (6 in. × 6 in. × 20 in.) tested over a span of 450 mm (18 in.). The standard beam is suitable for concrete containing aggregate with a nominal maximum size not exceeding 40 mm.

Non-Standard Small Prisms

When the available concrete volume or aggregate size permits, smaller beams of 100 mm × 100 mm × 400 mm may be used for concrete with aggregate not larger than 31.5 mm. Because smaller specimens exhibit a size effect, GB/T 50081 requires the measured flexural strength of 100 mm beams to be multiplied by a size conversion factor of 0.85 to obtain the equivalent standard value.

Fiber-Reinforced Concrete Beams

For steel or macro-synthetic fiber-reinforced concrete, flexural performance is evaluated using notched or unnotched beams under standards such as ASTM C1609 or EN 14651. These tests record the full load–deflection curve to determine residual flexural strength and toughness in addition to the peak modulus of rupture.

Curing and Testing Age

Specimens shall be cast from the sampled fresh concrete in steel or rigid molds, demolded after 24 hours, and cured in a standard curing room at 20 ± 2 °C with a relative humidity of at least 95%, or in lime-saturated water. Unless otherwise specified, testing is performed at the design age, commonly 28 days, with the time tolerance stipulated by the applicable standard.

Testing Items

The flexural strength test program typically includes the following determined parameters:

  • Peak failure load of the beam specimen (recorded in kN)
  • Flexural strength, or modulus of rupture, calculated in MPa (N/mm²)
  • Failure location and fracture pattern within the constant-moment zone
  • Load–deflection response and residual flexural strength (for fiber-reinforced concrete)
  • Conversion of non-standard specimen results to standard-size equivalence
  • Statistical evaluation of a set of three companion specimens, including mean and median values

Testing Methods

Apparatus Requirements

The test requires a compression testing machine of sufficient capacity and verified accuracy (typically Class 1 or better), fitted with a dedicated flexural loading attachment. The fixture consists of two support rollers spaced at the test span and two loading rollers positioned at the third points of the span, each able to rotate slightly to maintain contact. Dimensional measurements are taken with a vernier caliper or steel rule readable to 1 mm. A damp cloth is used to wipe the specimen surface before testing.

Step-by-Step Test Procedure

  • Step 1 – Remove the specimen from the curing room and allow it to reach a surface-dry condition; wipe away free moisture and surface debris. Test the specimen as soon as practicable after removal from curing.
  • Step 2 – Measure the width (b) and height (h) of the beam at the mid-span cross-section, taking measurements at multiple locations and averaging them to the nearest 1 mm. Confirm that the specimen is free of visible cracks, honeycombing, or edge defects that would invalidate the result.
  • Step 3 – Mark the mid-span and the two third-point positions on the tension (bottom) face of the beam to assist with alignment of the loading rollers.
  • Step 4 – Install the flexural attachment on the testing machine and set the support span (450 mm for standard specimens). Align the fixture so that the loading axis passes vertically through the centroid of the beam cross-section.
  • Step 5 – Place the specimen on the supports with the casting position oriented so that the direction of loading is perpendicular to the direction of casting, and align the two loading rollers exactly over the marked third points, each 150 mm from the supports and from each other.
  • Step 6 – Bring the loading head into contact with the beam, apply a small initial seating load, and zero the load indicator.
  • Step 7 – Apply the load continuously and uniformly without shock at a constant rate specified by the governing standard (for example, approximately 0.02–0.05 MPa/s under GB/T 50081), until the specimen fails. Do not adjust or interrupt the loading at any point during the test.
  • Step 8 – Record the maximum failure load, the location of the fracture, and the fracture pattern immediately after failure.
  • Step 9 – Repeat the procedure for all three companion specimens in the test set.

Calculation of Flexural Strength

For third-point loading, the flexural strength is calculated as the moment divided by the section modulus of a rectangular section, using the formula:

f = F × L / (b × h²)

where f is the flexural strength in MPa, F is the peak failure load in newtons, L is the support span (450 mm), and b and h are the measured width and height of the specimen in millimeters. The result is reported to the precision required by the applicable standard, commonly to the nearest 0.01 MPa under GB/T 50081. For center-point loading per ASTM C293, the formula becomes f = 3FL / (2bh²), which yields characteristically higher values because the maximum moment occurs at a single critical section.

Result Validity and Data Reduction

  • A fracture occurring within the middle third of the span (between the two loading points) is considered valid, since this zone is under pure bending without shear.
  • If the fracture occurs outside the middle third or close to a support, the result is rejected or treated according to the specific provisions of the governing standard.
  • For a set of three specimens, the flexural strength is taken as the arithmetic mean. If the maximum or minimum value deviates from the median by more than 15%, the median is adopted; if both extreme values exceed this limit, the entire set is discarded and the test repeated.
  • Results from 100 mm non-standard beams must be multiplied by the size conversion factor (0.85) before being compared with specified standard values.

Applications

Flexural strength test results are applied across a wide range of civil engineering and infrastructure contexts:

  • Design and acceptance of rigid (jointed plain and continuously reinforced) concrete pavements for highways and expressways, where the modulus of rupture is the primary design parameter
  • Quality control and mix proportioning verification for airport runways, taxiways, and apron pavements subject to heavy aircraft wheel loads
  • Evaluation of industrial floors, warehouse slabs, and slab-on-grade systems where bending stress governs performance
  • Assessment of fiber-reinforced concrete toughness and post-cracking residual capacity for shotcrete, tunnel linings, and precast segments
  • Comparative evaluation of supplementary cementitious materials, admixtures, and curing regimes on concrete tensile performance
  • Structural research, finite element model calibration, and compliance verification in accredited third-party laboratories and ready-mix concrete plants

FAQ

What is the difference between flexural strength and compressive strength?

Compressive strength measures the resistance of concrete to crushing loads and is tested on cubes or cylinders, while flexural strength measures resistance to bending failure and is tested on beams. Flexural strength is directly related to the tensile capacity of concrete and is typically only a fraction of compressive strength, usually 10% to 20% depending on the mix, aggregate type, and curing quality.

Can 100 mm beams be used instead of standard 150 mm beams?

Yes, provided the nominal maximum aggregate size does not exceed 31.5 mm and the concrete volume is limited. However, because smaller beams show a size effect, the measured flexural strength must be multiplied by a conversion factor of 0.85 under GB/T 50081 to obtain the equivalent standard specimen value.

Why is third-point loading preferred over center-point loading?

Third-point loading creates a region of constant maximum bending moment with zero shear between the two loading points, so failure occurs at the weakest point within that zone and better represents the true tensile strength of the material. Center-point loading concentrates the maximum moment at a single cross-section, which often produces higher and more variable results.

What loading rate should be used during the test?

The load must be applied continuously and uniformly without shock at the constant rate specified by the governing standard, for example approximately 0.02–0.05 MPa/s for ordinary concrete under GB/T 50081. Using an incorrect rate can significantly bias the measured strength, with faster rates producing higher apparent values.

How is flexural strength related to compressive strength?

Empirical relationships, such as expressions in ACI and other national design codes that relate the modulus of rupture to the square root of compressive strength, can be used for estimation. However, because flexural strength is highly sensitive to aggregate type, moisture condition, and curing, direct beam testing remains essential whenever flexural strength is a specified acceptance criterion.

What happens if the beam breaks outside the middle third?

A fracture outside the middle third of the span indicates that failure was influenced by shear or local effects rather than pure bending, so the result is generally rejected. The specific acceptance rules for such fractures, including cases where the anomalous result is not lower than the remaining valid values, are defined in the applicable standard such as ASTM C78 or GB/T 50081.

Why Choose ZKGX?

  • State-of-the-art analytical equipment
  • Highly qualified scientific team
  • Fast turnaround time
  • Competitive pricing